Low alloy tuang baja nujul kana alloy tuang baja kalawan eusi karbon kirang ti 0,45% sarta eusi total elemen alloying séjén teu ngaleuwihan 5%. Low alloy tuang baja boga kakuatan tinggi, kateguhan alus tur hardenability. Low alloy tuang baja umumna ngandung elemen alloying kayaning mangan, kromium, tambaga, nikel, molybdenum, sarta vanadium. Aranjeunna gaduh kateguhan dampak anu langkung ageung sareng tiasa nampi sipat mékanis anu langkung saé ngalangkungan perlakuan panas. Résistansi korosi sareng tahan ngagem tina baja tuang alloy low langkung saé tibatan baja karbon, anu tiasa ngirangan beurat bagian sareng ningkatkeun umur jasa.
Sasmita jeung Komposisi Kimia Low alloy tuang Steel | |||||||||
Kelas | C (%) | Si (%) | Mn (%) | P≦ (%) | S≦ (%) | Cr (%) | Ni (%) | Mo (%) | Cu≦ (%) |
ZG20Mn | 0.16~0.22 | 0.6~0.8 | 1.00 ~ 1.30 | 0.03 | 0.03 | —— | ≦0.4 | —— | —— |
ZG30Mn | 0.27~0.34 | 0.30~0.50 | 1.20 ~ 1.50 | 0.03 | 0.03 | —— | —— | —— | —— |
ZG35Mn | 0.30~0.40 | 0,60 ~ 0,80 | 1.10~1.40 | 0.03 | 0.03 | —— | —— | —— | —— |
ZG40Mn | 0.35~0.45 | 0.30~0.45 | 1.20 ~ 1.50 | 0.03 | 0.03 | —— | —— | —— | —— |
ZG40Mn2 | 0.35~0.45 | 0.20~0.40 | 1.60~1.80 | 0.03 | 0.03 | —— | —— | —— | —— |
ZG45Mn2 | 0.42~0.49 | 0.20~0.40 | 1.60~1.80 | 0.03 | 0.03 | —— | —— | —— | —— |
ZG50Mn2 | 0,45 ~ 0,55 | 0.20~0.40 | 1.50~1.80 | 0.03 | 0.03 | —— | —— | —— | —— |
ZG35SiMnMo | 0.32~0.40 | 1.10~1.40 | 1.10~1.40 | 0.03 | 0.03 | —— | 0.20~0.30 | 0.3 | |
ZG35CrMnSi | 0.30~0.40 | 0,50 ~ 0,75 | 0.90~1.20 | 0.03 | 0.03 | 0,50~0,80 | —— | —— | —— |
ZG20MnMo | 0.17~0.23 | 0.20~0.40 | 1.10~1.40 | 0.03 | 0.03 | —— | —— | 0.20~0.35 | 0.3 |
ZG30Cr1MnMo | 0.25~0.35 | 0.17~0.45 | 0.90~1.20 | 0.03 | 0.03 | 0.90~1.20 | 0.20~0.30 | —— | |
ZG55CrMnMo | 0.50~0.60 | 0,25 ~ 0,60 | 1.20~1.80 | 0.03 | 0.03 | 0.60~0.90 | —— | 0.20~0.30 | 0.3 |
ZG40Cr1 | 0.35~0.45 | 0.20~0.40 | 0,50~0,80 | 0.03 | 0.03 | 0.80~1.10 | —— | —— | —— |
ZG34Cr2Ni2Mo | 0.30~0.37 | 0.30~0.60 | 0.60~1.00 | 0.03 | 0.03 | 1.40~1.70 | 1.40~1.70 | 0.15~0.35 | —— |
ZG15Cr1Mo | 0.12~0.20 | 0.6 | 0,50~0,80 | 0.03 | 0.03 | 1.00 ~ 1.50 | —— | 0,45 ~ 0,65 | —— |
ZG20CrMo | 0.17~0.25 | 0.20~0.45 | 0,50~0,80 | 0.03 | 0.03 | 0,50~0,80 | —— | 0,45 ~ 0,65 | —— |
ZG35Cr1Mo | 0.30~0.37 | 0.30~0.50 | 0,50~0,80 | 0.03 | 0.03 | 0.80~1.20 | —— | 0.20~0.30 | —— |
ZG42Cr1Mo | 0.38~0.45 | 0.30~0.60 | 0.60~1.00 | 0.03 | 0.03 | 0.80~1.20 | —— | 0.20~0.30 | —— |
ZG50Cr1Mo | 0.46~0.54 | 0,25 ~ 0,50 | 0,50~0,80 | 0.03 | 0.03 | 0.90~1.20 | —— | 0.15~0.25 | —— |
ZG65Mn | 0.60~0.70 | 0.17~0.37 | 0.90~1.20 | 0.03 | 0.03 | —— | —— | —— | —— |
ZG28NiCrMo | 0.25~0.30 | 0.30~0.80 | 0.60~0.90 | 0.03 | 0.03 | 0.35~0.85 | 0.40~0.80 | 0,35 ~ 0,55 | —— |
ZG30NiCrMo | 0.25~0.35 | 0.30~0.60 | 0.70 ~ 1.00 | 0.03 | 0.03 | 0.60~0.90 | 0.60~1.00 | 0,35 ~ 0,50 | —— |
ZG35NiCrMo | 0.30~0.37 | 0.60~0.90 | 0.70 ~ 1.00 | 0.03 | 0.03 | 0.40~0.90 | 0.60~0.90 | 0,40 ~ 0,50 | —— |
Sipat mékanis tina baja tuang alloy low | |||||||||
Kelas | perlakuan panas | Kakuatan ngahasilkeun Rp0.2/Mpa (≧) | Kakuatan Tensile Rm/Mpa (≧) | A(%) ≧ | Z(%) ≧ | KU2/J ≧ | KV2/J ≧ | AKDVM/J ≧ | Teu karasa HBW |
ZG20Mn | Normalisasi + Tempering | 285 | 495 | 18 | 30 | 39 | —— | —— | 145 |
Quenching + Tempering | 300 | 500~650 | 24 | —— | —— | 45 | —— | 150~190 | |
ZG30Mn | Normalisasi + Tempering | 300 | 558 | 18 | 30 | —— | —— | —— | 163 |
ZG35Mn | Normalisasi + Tempering | 345 | 570 | 12 | 20 | 24 | —— | —— | —— |
Quenching + Tempering | 415 | 640 | 12 | 25 | 27 | —— | 27 | 200~240 | |
ZG40Mn | Normalisasi + Tempering | 295 | 640 | 12 | 30 | —— | —— | —— | 163 |
ZG40Mn2 | Normalisasi + Tempering | 395 | 590 | 20 | 40 | 30 | —— | —— | 179 |
Quenching + Tempering | 685 | 835 | 13 | 45 | 35 | —— | 35 | 269~302 | |
ZG45Mn2 | Normalisasi + Tempering | 392 | 637 | 15 | 30 | —— | —— | —— | 179 |
ZG50Mn2 | Normalisasi + Tempering | 445 | 785 | 18 | 37 | —— | —— | —— | —— |
ZG35SiMnMo | Normalisasi + Tempering | 395 | 640 | 12 | 20 | 24 | —— | —— | —— |
Quenching + Tempering | 490 | 490 | 12 | 25 | 27 | —— | 27 | —— | |
ZG35Mn | Normalisasi + Tempering | 345 | 570 | 12 | 20 | 24 | —— | —— | —— |
Quenching + Tempering | 415 | 640 | 12 | 25 | 27 | —— | 27 | —— | |
ZG35CrMnSi | Normalisasi + Tempering | 345 | 690 | 14 | 30 | —— | —— | —— | 217 |
ZG20MnMo | Normalisasi + Tempering | 295 | 490 | 16 | —— | 39 | —— | —— | 156 |
ZG30Cr1MnMo | Normalisasi + Tempering | 392 | 686 | 15 | 30 | —— | —— | —— | —— |
ZG55CrMnMo | Normalisasi + Tempering | / | / | —— | —— | —— | —— | —— | —— |
ZG40Cr1 | Normalisasi + Tempering | 345 | 630 | 18 | 26 | —— | —— | —— | 212 |
ZG34Cr2Ni2Mo | Quenching + Tempering | 700 | 950~1000 | 12 | —— | —— | 32 | —— | 240~290 |
ZG15Cr1Mo | Normalisasi + Tempering | 275 | 490 | 20 | 35 | 24 | —— | —— | 140~220 |
ZG20CrMo | Normalisasi + Tempering | 245 | 460 | 18 | 30 | 30 | —— | —— | 135~180 |
Quenching + Tempering | 245 | 460 | 18 | 30 | 24 | —— | —— | —— | |
ZG35Cr1Mo | Normalisasi + Tempering | 392 | 588 | 12 | 20 | 23.5 | —— | —— | —— |
Quenching + Tempering | 510 | 686 | 12 | 25 | 31 | —— | 27 | 201 | |
ZG42Cr1Mo | Normalisasi + Tempering | 343 | 569 | 12 | 20 | —— | 30 | —— | —— |
Quenching + Tempering | 490 | 690~830 | 11 | —— | —— | —— | 21 | 200~250 | |
ZG50Cr1Mo | Quenching + Tempering | 520 | 740~880 | 11 | —— | —— | —— | 34 | 200~260 |
ZG65Mn | Normalisasi + Tempering | / | / | —— | —— | —— | —— | —— | —— |
ZG28NiCrMo | —— | 420 | 630 | 20 | 40 | —— | —— | —— | —— |
ZG30NiCrMo | —— | 590 | 730 | 17 | 35 | —— | —— | —— | —— |
ZG35NiCrMo | —— | 660 | 830 | 14 | 30 | —— | —— | —— | —— |
waktos pos: Sep-29-2024